EN 10219-1 Pipa Baja
Oct 23, 2023
EN 10219-1 Pipa Baja
EN 10219-1 Analisis Kimia Pipa Baja
|
Kualitas baja |
Jenis de-oksidasi a |
% berdasarkan massa, maksimum |
||||||
|
Nama baja |
Nomor baja |
C |
C |
Ya |
M N |
P |
S |
Catatan |
|
S235JRH |
1.0039 |
FF |
0,17 |
— |
1,40 |
0,040 |
0,040 |
0.009 |
|
S275J0H |
1.0149 |
FF |
0,20 |
— |
1,50 |
0,035 |
0,035 |
0,009 |
|
S275J2H |
1.0138 |
FF |
0,20 |
— |
1,50 |
0,030 |
0,030 |
— |
|
S355J0H |
1.0547 |
FF |
0,22 |
0,55 |
1,60 |
0,035 |
0,035 |
0,009 |
|
S355J2H |
1.0576 |
FF |
0,22 |
0,55 |
1,60 |
0,030 |
0,030 |
— |
|
S355K2H |
1.0512 |
FF |
0,22 |
0,55 |
1,60 |
0,030 |
0,030 |
— |

EN 10219-1 Sifat Mekanik Pipa Baja
| Kualitas baja | Baja No. | Peralatan mekanis | Energi Dampak (KV J) | ||||
| Kekuatan Hasil (Mpa) | Kekuatan Tarik (Mpa) | Perpanjangan (%) | Suhu Uji Pada Suhu Ujiderajat | ||||
| -20 | 0 | 20 | |||||
| S235JRH | 1.0039 | 235 | 360-510 | 26 | – | – | 27 |
| S275J0H | 1.0149 | 275 | 410-560 | 23 | – | 27 | – |
| S275J2H | 1.0138 | 275 | 410-560 | 23 | 27 | – | – |
| S355J0H | 1.0547 | 355 | 510-680 | 22 | – | 27 | – |
| S355J2H | 1.0576 | 355 | 510-680 | 22 | 27 | – | – |
| S355K2H | 1.0512 | 355 | 510-680 | 22 | 40 | – | – |
PERUSAHAAN GNEE